The manufacturing processes for Teflon-insulated wires primarily include paste extrusion, tape wrapping, and melt extrusion; the specific method chosen depends on the type of fluoroplastic used. Due to its extremely high melt viscosity, PTFE (polytetrafluoroethylene) cannot be processed via conventional screw extrusion; instead, it is typically applied through paste extrusion or film wrapping. In contrast, melt-processable fluoroplastics - such as FEP, PFA, and ETFE - are processed using melt extrusion.
Paste Extrusion Process (for PTFE)
This process is used for PTFE dispersion resins and is based on the principle of "cold-press extrusion followed by high-temperature sintering."
1. Preparation: PTFE dispersion resin powder is mixed with an extrusion aid (a liquid hydrocarbon) to form a paste, which is then pre-pressed into a "preform" (billet).
2. Extrusion Coating: The preform is placed into a paste extruder, where a piston applies a force of approximately 140 MPa. As the conductor passes through a hollow core die, the PTFE paste is forced through an extrusion die, coating the conductor uniformly. The extrusion speed is typically around 50 mm/min, with a die cone angle generally set at 20°.
3. Drying and Degreasing: The coated wire enters a drying oven to remove the extrusion aid; this stage requires a robust exhaust ventilation system.
4. High-Temperature Sintering: The wire then enters a sintering furnace, where it is heated to approximately 380°C. At this temperature, the PTFE particles melt and fuse together to form a continuous, solid insulating layer.
5. Cooling and Inspection: After cooling and setting, the wire undergoes a high-voltage spark test to ensure dielectric integrity before being spooled.
Key Parameters: The compression ratio is typically set between 300 and 800; this directly influences the density of the insulation and the risk of cracking. Furthermore, the extrusion speed must be carefully matched with the drying rate; otherwise, the insulation may discolor (turning yellow or black).
Tape Wrapping Process (for PTFE)
This process is used for thin films (tapes) derived from PTFE suspension resins.
1. Film Production: PTFE produced via suspension polymerization is molded and sintered into a billet, which is then skived (peeled) and rolled into an oriented film. The degree of orientation is selected based on the required insulation thickness.
2. Tape-Wrapping: The film is cut into narrow strips and wrapped in multiple layers around the conductor core.
3. Sintering and Setting: Following the wrapping process, the cable undergoes high-temperature sintering. The shrinkage - a result of the film's molecular orientation - causes the layers to fuse tightly together.
4. Inspection: Includes spark testing (dielectric withstand testing) and final product inspection.
Thermal Extrusion Process (for FEP/PFA/ETFE)
Used for melt-processable fluoroplastics; the process is similar to standard plastic extrusion, though it requires more stringent temperature control.
1. Preheating: FEP resin is pre-dried at 120°C for approximately 3 hours. The conductor is preheated to a temperature between 150°C and 350°C (depending on the specific material) to prevent internal stress caused by the rapid cooling of the molten plastic.
2. Extrusion: The temperature along the extruder barrel increases linearly from approximately 280°C at the feed inlet to 380°C at the die head, with the die sleeve maintained between 380°C and 410°C. A sleeve-type (tubing) die is used, with a draw-down ratio typically ranging from 50 to 200, and a draw-balance coefficient controlled between 0.9 and 1.15.
3. Cooling: A multi-stage cooling approach is employed, with water bath temperatures set in a descending gradient - starting at approximately 70°C - to avoid rapid cooling, which could otherwise lead to a loose-fitting insulation layer or the development of internal stress.
4. In-line Inspection: The process incorporates comprehensive monitoring, including outer diameter (OD) feedback, spark testing, and water-immersion capacitance testing.